Balance Community Materials test laboratory · SnapLab

Record Sample 1
Product Secondaire MK2
Batch W26AC

Tensile test

Sample 1

Secondaire MK2Batch W26ACJuly 23, 2026

Breaking force

24.42kN

Force–time trace

The capture from the rig’s force channel, plotted against elapsed time.

Test details

Tested
Jul 23, 2026 · 16:44
Duration
138.8s
Scan rate
500.0Hz
Sample
1
Study
Batch Report - Secondaire MK2 - W26AC
Test machine
SnapLab break-test bench
DAQ device
LabJack T7
Beam location
No. 2 — Second position
Fixed grip
Sewn Loop
Moving grip
Sewn Loop

Instrumentation

Recorded channels
Channel Sensor Type Units Calibrated
AIN2 Main Main Force Sensor force kN Not recorded

Method

Secondaire MK2 sewn loop (pattern 504) in the Sewn Loop to Sewn Loop break-test rig, line drawing

Drag to rotate · scroll or pinch to zoom · right-drag or two-finger drag to pan

Test setup: Sewn Loop to Sewn Loop · Diamond ramp for 20 mm webbings

Configuration Sewn Loop to Sewn Loop

Sewing pattern Diamond ramp for 20 mm webbings Pattern 504

Determines strength retention in a sewn loop. The particular pattern used for sewing is indicated on each test.

Each sewn loop is done in an opposite direction in order to take out the possibility of failure by uneven loading across the width and thickness of the webbing. Each sewn loop is directly attached to the clevis pins on our test machine, with a diameter of pin diameter of 19mm.

These tests are often used as our elongation tests as well, since they experience the least change in length within the anchoring method.

  • Webbing starting length - 1.5 m (5 ft)

  • Pull Rate - ~350 mm per minute

Part of batch W26AC →